改性煤矸石对味精废水的吸附试验研究

 
改性煤矸石对味精废水的吸附试验研究

改性煤矸石对味精废水的吸附试验研究

摘要:利用煤矸石中碳、硅、铝共存的特性,对其进行改性,可制备出吸附性能优良的吸附剂,为工业废水和中水回用的吸附处理提供新材料。本研究通过改性煤矸石对味精废水进行吸附实验,探讨改性煤矸石的粒径、用量、吸附时间对味精废水的氨氮, COD吸附的影响。 结果表明,改性煤矸石的粒径为120目,吸附时间180min、投加量4.0g时,对味精废水COD和氨氮去除率最大。

关键词:改性煤矸石;吸附;味精废水; 去除率

Abstract: by using coal gangue, silicon, aluminum carbon in the characteristics of coexistence, and carry on the modification, can be prepared by the good performance of absorbent adsorption, for industrial waste water and water reuse adsorption deal with new material. This study through the modification of coal gangue monosodium glutamate wastewater for adsorption experiment, this paper discusses the size and amount of the modified coal gangue, adsorption time on the monosodium glutamate wastewater ammonia nitrogen, COD adsorption effect. The results showed that the modification gangue particle size of 120 mesh, adsorption time 180 min, dosing quantity 4.0 g, monosodium glutamate wastewater of COD and ammonia nitrogen removal efficiency is the largest.

Keywords: modified coal gangue; Adsorption; Monosodium glutamate wastewater; Removal rate

煤矸石是煤矿开采、洗选加工过程中产生的废石。随着科学的发展,人们逐渐认识到煤矸石也是可利用的一种资源。研究证明,煤矸石作为原材料广泛用于化工、建筑、农业、电力、等行业。本研究通过试验模拟,描述不同粒径、不同投加量和吸附时间的煤矸石对味精废水COD和氨氮去除率的变化,探讨煤矸石用于吸附材料处理味精废水的可行性。

1 材料与方法

1.1改性煤矸石的制备

煤矸石取自于平顶山市煤矿,其化学组成比较复杂,SiO2和Al2O3,SiO2等相对含量在60%左右;另外,还有一些微量元素和稀土元素。X射线衍射测试结果表明,煤矸石主要以粘土矿物为主体,其中高岭石的相对含量高达60%~70%左右,另外含有一些蒙脱石、伊利石、石英、白云石和方解石等。

将煤矸石与ZnC12按一定比例混匀,高温下煅烧一定时间,室温下冷却,取一定量样品用一定浓度的HCl加热回流酸化2h,水洗至pH值为中性,105℃下干燥,即得改性煤矸石[1]。

1.2 样品制备